For what its worth - all of the filaments I stored in the cereal containers with silica gel with the hygrometers back in APRIL are still happily reporting 10% RH. I don't see any reason why that would change unless the containers are open.
There's a lot of chatter about filament moisture content out there, but be realistic - the printed plastic is also subject to moisture absorption, so if you are interested in the real material properties and final stiffness/strength properties, these should be measured some time after printing, when the humidity has stabilized.
Nylon 6 and Nylon 12 alloys are really the only materials I have had problems with while printing, but only when the material humidity seems to be high (e.g. 20% or more). Nylons really do need to be quite dry before printing. And when printing, the correct bed adhesive is essential. The usual glue sticks simply do not work, so a PA specific adhesive is needed. These adhesives work well if the filament is dry, but always fail if the filament is wet, so keep that in mind.
PET and PETG are not nearly as sensitive to filament moisture as Nylons and can be printed on a clean bed plate even if the humidity is slightly elevated.
Polycarbonate can fizz and bubble at the nozzle if it is wet (15% or more), and PLA is (from the print quality perspective) is mostly unaffected by moisture content unless it is saturated, despite what the "influencers" promoting dryer gadgets would want you to believe.
Yep, I recognize the need for science in this subject, but it is the final print and long term structural performance that actually matter.
I have been manufacturing 3D printed machine components for quite a while now, with many parts incorporated into production machines that have seen many years of service. I am not aware of any run-time failures due to humidity affected components if they are correctly designed.
There's a lot of chatter about filament moisture content out there, but be realistic - the printed plastic is also subject to moisture absorption, so if you are interested in the real material properties and final stiffness/strength properties, these should be measured some time after printing, when the humidity has stabilized.
Nylon 6 and Nylon 12 alloys are really the only materials I have had problems with while printing, but only when the material humidity seems to be high (e.g. 20% or more). Nylons really do need to be quite dry before printing. And when printing, the correct bed adhesive is essential. The usual glue sticks simply do not work, so a PA specific adhesive is needed. These adhesives work well if the filament is dry, but always fail if the filament is wet, so keep that in mind.
PET and PETG are not nearly as sensitive to filament moisture as Nylons and can be printed on a clean bed plate even if the humidity is slightly elevated.
Polycarbonate can fizz and bubble at the nozzle if it is wet (15% or more), and PLA is (from the print quality perspective) is mostly unaffected by moisture content unless it is saturated, despite what the "influencers" promoting dryer gadgets would want you to believe.
Yep, I recognize the need for science in this subject, but it is the final print and long term structural performance that actually matter.
I have been manufacturing 3D printed machine components for quite a while now, with many parts incorporated into production machines that have seen many years of service. I am not aware of any run-time failures due to humidity affected components if they are correctly designed.